Injection molding defects are rarely random. Most recurring quality problems trace back to one of three places: part design, process settings, or material behavior. The challenge for engineering and quality teams is that a visible defect often has more than one plausible root cause, so the fastest path to a permanent fix is a structured design-for-manufacturing review rather than trial and error on the press.
This guide covers 12 of the most common defects found during development and production launches: sink marks, flash, warpage, weld lines, short shots, burn marks, flow lines, splay, jetting, voids, delamination, and ejector marks. For the six defects that most often block cosmetic approval or stable launch readiness, the guide also includes custom visuals that show what the failure looks like and what a better design strategy looks like.
Use this article as a practical field reference during Phase 0 design reviews, mold trials, and T0/T1/T2 gate meetings. The goal is not just to identify defects faster, but to create a repeatable decision path for solving them at the source.
Quick Reference: 12 Common Injection Molding Defects
| Defect | What it looks like | Check first | Typical first fix |
| Sink marks | Surface depressions over thick sections | Design | Core out thick areas and reduce rib/boss thickness |
| Flash | Thin fins at parting lines or shutoffs | Design / Process | Add shutoff draft and reduce overpacking |
| Warpage | Twist, bow, or saddle shape | Design / Process | Balance walls, gates, and cooling |
| Weld lines | Visible lines where flow fronts meet | Design / Process | Move convergence off cosmetic faces |
| Short shots | Incomplete fill or unfilled ribs | Design / Process | Increase flow capability and gate size |
| Burn marks | Black or brown marks at end of fill | Design / Tooling | Add vents at last-fill zones |
| Flow lines | Wavy streaks or gloss bands | Process | Optimize speed and temperature profile |
| Splay | Silvery streaks from the gate | Material / Process | Dry resin and reduce shear |
| Jetting | Snake-like streamers from gate | Design / Process | Use fan or tab gates and reduce initial speed |
| Voids | Internal air pockets near thick sections | Design / Process | Core sections and extend hold/cooling |
| Delamination | Surface layers peel or flake | Material / Process | Eliminate contamination and moisture |
| Ejector marks | White marks or pin witness damage | Design / Process | Increase draft and improve ejection support |
Defect 1: Sink Marks
Sink marks appear as shallow surface depressions, usually above a thick boss, heavy rib, or abrupt wall transition. The defect is caused by volumetric shrinkage. The interior mass of the part stays molten longer than the skin, so as the part cools and shrinks, it pulls the outer wall inward.
The most reliable way to prevent sink marks is to control geometry before the tool is built. Core out bosses whenever possible, keep boss outside diameter at or below about twice the nominal wall, and target rib thickness around 50 to 60 percent of the main wall. Sudden thickness changes should taper gradually. If the part is cosmetic, a matte or textured finish can reduce visibility, but finish should not be treated as the primary fix.
On the process side, hold pressure and hold time can help, but they cannot completely rescue a part with excessive mass concentration. If sink remains after process optimization, the design is usually the primary lever.
Defect 2: Flash
Flash is excess material that escapes at the parting line, ejector pin holes, shutoffs, or vent gaps. It often looks like a thin fin of plastic that must be trimmed away, but on cosmetic surfaces it can immediately cause rejection.
Flash can come from several sources at once: flat shutoffs with no draft, parting lines placed on broad cosmetic faces, overpacking, excessive melt temperature, low-viscosity material, or a worn tool. The design fix is to add 3 to 5 degrees of shutoff draft where needed, place the parting line on a sharper edge break, and create a tear-strip moat around the area so any residual flash becomes easier to control and remove.
During trials, verify that clamp force is appropriate for the projected area and cavity pressure. If flash shows up only at higher pack, it may be a process symptom. If it appears persistently at a specific edge, the mold geometry or wear condition is more likely.
Defect 3: Warpage
Warpage is the large family of dimensional distortions that includes bowing, twisting, and saddle-shaped parts. The root cause is uneven shrinkage. That uneven shrinkage may come from wall variation, asymmetric ribbing, unbalanced gate strategy, different mold temperatures across the part, or resin behavior such as shrink anisotropy in semi-crystalline or filled materials.
A practical first question is whether the design is balanced. Long parts with a single end gate often twist because one side of the fill path freezes differently from the other. Large trays or covers with ribs concentrated on one side often bow. Good warpage prevention usually starts with uniform walls within about plus or minus 10 percent, symmetric geometry where possible, multiple or opposing gates for long parts, and cooling circuits that remove heat evenly.
Process adjustments can reduce warp, but balanced geometry and cooling are the long-term cure. If flatness is critical, conformal or well-balanced cooling is often worth the extra tooling effort.
Defect 4: Weld or Knit Lines
Weld lines form where two or more flow fronts meet. Sometimes the result is purely cosmetic. In other cases, the weld line becomes a structural weak point, especially in filled or semi-crystalline materials. The most painful version is a weld line running across an A-surface or through a high-stress feature.
The cleanest strategy is to control where convergence happens. Reduce unnecessary gate count, avoid placing holes and bosses in the main flow path unless needed, add overflow tabs where fronts can meet off the cosmetic face, and vent the convergence zone so trapped air can escape. Rounded internal corners also help by reducing hesitation and improving fill balance.
From a materials standpoint, amorphous resins such as ABS, PC, and PMMA typically fuse better at the interface than crystalline families. If the material is fixed, higher melt and mold temperatures and a faster fill can improve weld strength by keeping the fronts hot when they meet.
Defect 5: Short Shots
Short shots happen when the cavity does not fill completely. In development, the easiest clues are unfilled ribs, thin sections that never complete, or a cavity that stalls before the end of fill. While low pressure or low temperature can cause the symptom, the design often sets the trap by demanding more flow length than the resin can realistically deliver.
A useful rule of thumb is to respect flow-length-to-wall-thickness limits and avoid extremely thin sections unless the geometry and material are designed for it. Commodity resins often need at least about 0.8 mm wall, while engineering materials are safer at 1.2 mm and above. Gate diameter should generally be at least 0.8 times the nominal wall, and venting should be added at regular intervals and at end-of-fill regions.
If the design is already steel-cut, process adjustments such as higher injection speed, higher melt temperature, and a larger gate can help. But if the part routinely stalls in thin long features, design simplification or a higher-flow grade may be the better solution.
Defect 6: Burn Marks
Burn marks, also called dieseling, are black or brown marks created when trapped air compresses and ignites at the end of fill. They usually appear at rib tips, deep bosses, dead-end flow paths, or any last-fill location that does not vent well.
The fix begins with vent strategy. Identify the actual last-fill zones through Moldflow, short-shot study, or experience from the press, then place vents there. Rib tips and boss tops often need micro-vents. Internal corners should be radiused where possible so air does not become trapped in stagnant pockets.
Process changes can help if the tool is close to acceptable. Slower multi-stage fill, slightly lower melt temperature, and regular vent cleaning all reduce the chance that air reaches ignition conditions. Moisture in the resin can make the problem worse, so material drying should always be verified when burn marks appear.
Additional Defects to Watch
Flow lines
Wavy or streaked surface patterns caused by abrupt wall changes, poor gate geometry, or an inconsistent speed profile. Start by raising mold or melt temperature, optimizing the fill profile, and rounding corners.
Splay or silver streaks
Silvery streaks radiating from the gate usually point to moisture, gas, or shear. Dry hygroscopic materials to spec, reduce screw RPM, and enlarge overly small gates that over-shear the melt.
Jetting
Snake-like streamers occur when a small gate shoots a high-velocity stream into open space. Fan or tab gates, a short gate land, an impinging wall, and a slower initial speed usually correct it.
Voids
Internal air pockets near thick regions are common when hold pressure is insufficient or the gate freezes early. Core thick sections, increase hold time, and verify the gate does not freeze too soon.
Delamination
Peeling surface layers often indicate contamination, incompatible regrind, or moisture. Purge thoroughly, reduce mold release use, and verify resin compatibility and dryness.
Ejector marks
White stress marks or pin witness damage appear when the part grips the core or ejects too hot. Increase draft, add ejector pads, extend cooling, and consider stripper plate or air eject for delicate geometries.
Defect Origin Matrix: Where to Look First
| Defect | Design first? | Process first? | Material first? |
| Sink marks | Yes | Yes | |
| Flash | Yes | Yes | |
| Warpage | Yes | Yes | Yes |
| Weld lines | Yes | Yes | Yes |
| Short shots | Yes | Yes | Yes |
| Burn marks | Yes | Yes | |
| Flow lines | Yes | Yes | |
| Splay | Yes | Yes | |
| Jetting | Yes | Yes | |
| Voids | Yes | Yes | Yes |
| Delamination | Yes | Yes | |
| Ejector marks | Yes | Yes | Yes |
12-Point T0 / T1 / T2 Defect Gate
At each trial stage, every defect should be rated pass, fail, or hold with objective evidence. This prevents teams from debating subjective impressions and creates a clear escalation path from first shots to PPAP-ready production.
| Gate | Must pass | Evidence required |
| T0 | Short shots, flash, and major sink issues must be understood and contained. | Shot photos, part weights, basic cycle data |
| T1 | Cosmetic defects on A-surfaces must be reduced to target acceptance. | Visual standard, CMM data, appearance review notes |
| T2 | Zero critical defects, CTQ capability at target, and readiness for controlled production. | FAI, Cpk/SPC, control plan, PPAP-supporting records |
FAQ
What are the most common injection molding defects? The most common issues are sink marks, flash, warpage, weld lines, short shots, burn marks, flow lines, splay, jetting, voids, delamination, and ejector marks.
How do I tell sink marks from voids? Sink marks are visible surface depressions over heavy sections. Voids are internal pockets and may not show on the surface unless the part is sectioned or inspected with another method.
What causes flash at the parting line? Common causes include insufficient clamp force, worn or damaged parting line surfaces, zero-draft shutoffs, overpacking, and low-viscosity resin.
How do you fix weld lines on cosmetic surfaces? Move the convergence off the cosmetic face using single gating where possible, overflow tabs, better venting, and process settings that keep the flow fronts hotter when they meet.
Download the Injection Molding Defect Field Guide, or book a T0/T1/T2 gate review with Jaycon. If sink, flash, warp, or short shots are blocking approval, a focused DFM review usually identifies the highest-leverage change faster than trial-and-error process tuning.
Related reading
Get a DFM review with your quote. Upload a STEP file and get tooling and piece pricing back along with the design changes that reduce defect risk before you cut steel. Start a quote.